Bullseye Fuchsia Transparent Double Rolled 3 mm Glass
This style may not reveal (or strike to) its target color until fired.
Bullseye “Striker” Fusing Instructions
Some gold-bearing striking glasses, like this one, should be fired with a 2 hour hold at 1225°F during the initial stages of the firing cycle. If fired without this hold, they may not strike at all, or they may strike but appear spotty and have a blue-brown cast, as opposed to the desired target color. This full-fuse schedule effectively strikes these glasses:
Rate |
Temp |
Hold |
* |
1225 |
2:00 |
600 |
1490 |
:10 |
9999 |
900 |
** |
* The initial rate of heat is not a critical factor in successfully striking gold-bearing glasses. Choose an initial rate of heat appropriate to the scale and design of the project that you are firing.
** Remainder of cycle depends on the thickness of the piece. Consult the Bullseye Annealing Chart. For color-sensitive projects, we recommend testing the cycle you plan to use by fusing a small sample of a similar setup in the same kiln as the project to best predict final color results.
Compliments of A&A Products LLC